Synthesis, surface tension, optical and dielectric properties of bismuth oxide thin film
oraz
10 mar 2017
O artykule
Data publikacji: 10 mar 2017
Zakres stron: 87 - 93
Otrzymano: 21 lis 2015
Przyjęty: 03 sty 2016
DOI: https://doi.org/10.1515/msp-2017-0020
Słowa kluczowe
© 2017 Fatma Meydanerİ Tezel, İ. Afşin Kariper
This article is distributed under the terms of the Creative Commons Attribution Non-Commercial License, which permits unrestricted non-commercial use, distribution, and reproduction in any medium, provided the original work is properly cited.


![Transmittance T [%] and reflectivity R [%] of Bi2O2.75 thin film versus wavelength.](https://sciendo-parsed.s3.eu-central-1.amazonaws.com/647250fc215d2f6c89dc3e5d/j_msp-2017-0020_fig_003.jpg?X-Amz-Algorithm=AWS4-HMAC-SHA256&X-Amz-Content-Sha256=UNSIGNED-PAYLOAD&X-Amz-Credential=AKIA6AP2G7AKOUXAVR44%2F20250909%2Feu-central-1%2Fs3%2Faws4_request&X-Amz-Date=20250909T060555Z&X-Amz-Expires=3600&X-Amz-Signature=553e8937e01e00d93202062c8cdc7e818bb4f6ee74e19bc07f98b9e80288446d&X-Amz-SignedHeaders=host&x-amz-checksum-mode=ENABLED&x-id=GetObject)





Surface tension of test liquids used in the experiments_
Liquid | γ [mN/m] |
---|---|
Water | 72.8 |
Glycerin | 64 |
Ethylene glycol | 48 |
Iodometane | 35.27 |
Percentage elemental composition of the Bi2O2_75 thin film and bare glass_
Element | Bare glass | Bismuth oxide (Bi2O2.75) |
---|---|---|
Na | 9.02 | 5.14 |
Mg | 2.26 | 1.37 |
Al | 0.72 | 0.49 |
Si | 35.10 | 29.46 |
K | 0.21 | – |
Ca | 5.63 | 5.78 |
O | 47.06 | 19.21 |
Bi | – | 38.56 |
Contact angles of test liquids on Bi2O2_75 thin film_
Water | Glycerin | Ethylene glycol | Iodometane |
---|---|---|---|
78 | 63 | 52 | 9 |