Surface roughness analysis of prepolymerized CAD/CAM dental acrylic resins following combined surface treatments
, , , , , , et
14 oct. 2021
À propos de cet article
Publié en ligne: 14 oct. 2021
Pages: 209 - 218
Reçu: 03 mai 2021
Accepté: 17 août 2021
DOI: https://doi.org/10.2478/msp-2021-0018
Mots clés
© 2021 Afnan Alfouzan et al., published by Sciendo
This work is licensed under the Creative Commons Attribution-NonCommercial-NoDerivatives 4.0 International License.
Fig. 1

Fig. 2

Fig. 3

Pairwise comparison of the final surface roughness for the acrylic resins and disinfectants tested_
Group (I) | Comparison group (J) | Mean difference (I–J) | |
---|---|---|---|
Acrylic resins | |||
HC | CAD/CAM | 2.61 | 0.000 |
LC | 1.61 | 0.000 |
|
CAD/CAM | HC | −2.61 | 0.000 |
LC | −0.99 | 0.001 |
|
LC | HC | −1.61 | 0.000 |
CAD/CAM | 0.99 | 0.001 |
|
Disinfectants | |||
Corega | NaOCl | 0.41 | 0.328 |
CHG | −0.60 | 0.066 | |
NaOCl | Corega | −0.41 | 0.328 |
CHG | −1.01 | 0.000 |
|
CHG | Corega | 0.60 | 0.066 |
NaOCl | 1.01 | 0.000 |
Two-way repeated-measures ANOVA results for the interactions between resin type and disinfectants on the roughness values_
Source | Type III SS |
DF | MS | ||
---|---|---|---|---|---|
Corrected model | 145.99 | 8 | 18.24 | 18.45 | 0.000 |
Intercept | 235.61 | 1 | 235.61 | 238.28 | 0.000 |
Resin | 104.22 | 2 | 52.11 | 52.70 | 0.000 |
Disinfectants | 15.63 | 2 | 7.81 | 7.90 | 0.001 |
Resins×Disinfectants | 26.13 | 4 | 6.53 | 6.60 | 0.000 |
Error | 80.09 | 81 | 0.98 | ||
Total | 461.70 | 90 |
Mean surface roughness (Ra, μm) of the acrylic resins at baseline_
Acrylic resins | N | Mean ± SD | |
---|---|---|---|
HC | 30 | 0.24 ± 0.06 | <0.001 |
CAD/CAM | 30 | 0.03 ± 0.02 | |
LC | 30 | 0.17 ± 0.03 |