The Deposition Temperature Dependence on the Crystallite Size of NiO Thin Films

Publicado en línea: 15 Jun 2020
Volumen & Edición: Volumen 67 (2020) - Edición 1 (March 2020)
Páginas: 35 - 38
Recibido: 07 Jan 2020
Aceptado: 11 Feb 2020
Detalles de la revista
License
Formato
Revista
eISSN
1854-7400
Primera edición
30 Mar 2016
Calendario de la edición
4 veces al año
Idiomas
Inglés
Introduction

In previous years, the investigation of new materials for photovoltaic applications was dependent and related to the experimental and modelling parameters of any properties. Nickel oxide was obtained to belong in the group of semiconductor materials and is one of the best materials at present because of its good properties [1].

Nickel oxide (NiO) is a semiconductor material with a nature of p-type, which belonged to the part of TCO family. This attribute of NiO has several potential applications, for example, it is used in the gas sensors due to its band gap energy in the range of 3.6−4.0 eV and for the organic solar cells applications due to its p-type semiconducting [2]. It can be used in transparent diodes and even in the transparent transistors caused by the best optical transmission and electrical conductivity. Moreover, NiO can be used for defrosting windows due to its good conductivity, and fabricated NiO can be used in the UV photodetectors and touch screens due to its good responsivity [3, 4].

In the present article, we have studied and investigated a relationship to calculate the crystallite size (G) from the measured structural parameters of the X-ray diffraction in the NiO thin films. We have used the experimental data of NiO thin films prepared at several deposition temperatures in the range of 380–460°C [5], which present the following parameters, such as the diffraction angle 2θ, the full width at half-maximum (FWHM), the crystallite size G, the lattice parameter a and aa0 of (111) diffraction peak for NiO thin films at several deposition temperatures.

Materials and Methods

The NiO samples were fabricated on the glass substrates using a pneumatic spray technique with 0.1 M of the precursor molarity. The NiO thin films were deposited at several deposition temperatures in the range of 380–460°C [5] (see Table 1).

The diffraction angle 2θ, the full width at half-maximum (FWHM), the crystallite size G, the lattice parameter a and a − a0 of (111) diffraction peak for NiO thin films at several deposition temperatures [5].

Deposition temperature Ts (°C)2θ (deg)β (rad)G (nm)a (nm)aa0 (nm)
38037.800.0076619.130.41222810.00537184
40037.670.0078118.740.41358720.00401271
42037.640.0086816.880.41385300.00374695
44037.600.0079918.310.41434840.00325152
46037.660.0070720.720.41365070.00394921

Table 1 presents that the NiO thin films were nanocrystalline and had a cubic structure with (111) crystal plane at the higher intensity, which has preferential a-axis orientation along with (111) crystal plane.

The Miller indices (hkl) were obtained from the Bragg equation [6]: nλ=2dhklsinθn\lambda = 2{d_{hkl}}\,sin\,\theta where n, λ, dhkl and θ are the integers called the order of diffraction, the wavelength longer of X-ray (λ = 1.5406 A°), the interplanar spacing and the diffraction angle, respectively.

The lattice parameter a of cubic structure for NiO thin films was determined in Eq. (1) and XRD patterns using the following formula [5]: dhkl=ah+k+l{d_{h\,k\,l}} = {a \over {\sqrt {h + k + l}}}

The differences aa0 of (111) crystal plane are given by the following relation [6]: aa0=dhklh+k+la - {a_0} = {d_{hkl}}\sqrt {h + k + l} where a0 is the standard lattice parameter of NiO (standard a0 = 0.4176 nm). The crystallite size of (111) crystal plane for the fabricated NiO thin films was calculated from the Scherer's formula [7]: G=0.9λβcosθG = {{0.9\lambda} \over {\beta \,cos\,\theta}} where G is the experiment crystallite size, β is the FWHM and θ is the diffraction angle peak (see Table 1).

Results and Discussion

In this article, we have estimated the crystallite size (G) by fitting relationships between the structural parameters (β, a and aa0), which is detected in the following empirical relationship: G=C1aβC2aa0βG = {C_1}{a \over \beta} - {C_2}{{a - {a_0}} \over \beta} where C1 and C2 are constants as C1 = 0.365 and C2 = 0.02. The results of this fitting are given in Table 2.

The crystallite size G experimental and correlated at several deposition temperatures.

Deposition temperature Ts (°C)Experimental crystallite size (nm)Fitting crystallite size (nm)
38019.1319.14
40018.7418.84
42016.8816.96
44018.3118.45
46020.7220.82

Figure 1 shows the variation of the experimental and fitting of the crystallite size at several deposition temperatures in the range of 380–460°C. The measured values of the crystallite sizes were obtained using Eq. (5), which were given in Table 2. This correlation indicated that the crystallite sizes of the NiO thin films can be predominantly influenced by the FWHM β, the lattice parameter a and the differences in aa0 of the NiO thin films. As seen, all estimated values of crystallite sizes are proportional to the experimental data. Thus, the measurement of the crystallite size values by this proposed model is compatible with practical measurements qualitative. This attribution can be observed with the variation of FWHM β (see Figure 2). This observation was investigated to demonstrate that the calculation of the crystallite size can be influenced by the measurements of the structural parameters (β, a and aa0).

Figure 1

The variation of the crystallite size G experimental and fitting at several deposition temperatures.

Figure 2

The variation of the crystallite size G experimental and fitting at several FWHM values.

Conclusions

In this article, the direct correlation of the crystallite size from the experimental values was investigated by a fitting model wherein the calculated crystallite size of the pure NiO thin films was detected in the structural parameters, such as the FWHM β, the lattice parameter a and the differences in aa0. The experiment data of NiO thin films were prepared at several deposition temperatures in the range of 380–460°C. All estimated values of crystallite sizes are proportional to the experimental data. Thus, the measurement of the crystallite size values by this proposed model is compatible with practical measurements qualitative.

Figure 1

The variation of the crystallite size G experimental and fitting at several deposition temperatures.
The variation of the crystallite size G experimental and fitting at several deposition temperatures.

Figure 2

The variation of the crystallite size G experimental and fitting at several FWHM values.
The variation of the crystallite size G experimental and fitting at several FWHM values.

The crystallite size G experimental and correlated at several deposition temperatures.

Deposition temperature Ts (°C)Experimental crystallite size (nm)Fitting crystallite size (nm)
38019.1319.14
40018.7418.84
42016.8816.96
44018.3118.45
46020.7220.82

The diffraction angle 2θ, the full width at half-maximum (FWHM), the crystallite size G, the lattice parameter a and a − a0 of (111) diffraction peak for NiO thin films at several deposition temperatures [5].

Deposition temperature Ts (°C)2θ (deg)β (rad)G (nm)a (nm)aa0 (nm)
38037.800.0076619.130.41222810.00537184
40037.670.0078118.740.41358720.00401271
42037.640.0086816.880.41385300.00374695
44037.600.0079918.310.41434840.00325152
46037.660.0070720.720.41365070.00394921

Diha, A., Benramache, S., Benhaoua, B. (2018): Transparent nanostructured Co doped NiO thin films deposited by sol–gel technique. Optik, 172, pp. 832–839.DihaA.BenramacheS.BenhaouaB.2018Transparent nanostructured Co doped NiO thin films deposited by sol–gel techniqueOptik17283283910.1016/j.ijleo.2018.07.062Search in Google Scholar

Lamastra, F.R., Nanni, F., Menchini, F., Nunziante, P., Grilli, M.L. (2016): Transparent nanostructured electrodes: Electrospun NiO nanofibers/NiO films. Thin Solid Films, 601, pp. 54–58.LamastraF.R.NanniF.MenchiniF.NunzianteP.GrilliM.L.2016Transparent nanostructured electrodes: Electrospun NiO nanofibers/NiO filmsThin Solid Films601545810.1016/j.tsf.2015.09.019Search in Google Scholar

Hotovy, I., Spiess, L., Predanocy, M., Rehacek, V., Racko, J. (2014): Sputtered nanocrystalline NiO thin films for very low ethanol detection. Vacuum, 107, pp. 129–131.HotovyI.SpiessL.PredanocyM.RehacekV.RackoJ.2014Sputtered nanocrystalline NiO thin films for very low ethanol detectionVacuum10712913110.1016/j.vacuum.2014.04.012Search in Google Scholar

Ali, N., Hussain, A., Ahmed, R., Wang, M.K., Zhao, C., Haq, B.Ul., Fu, Y.Q. (2016): Advances in nanostructured thin film materials for solar cell applications. Renewable and Sustainable Energy Reviews, 59, pp. 726–737.AliN.HussainA.AhmedR.WangM.K.ZhaoC.HaqB.Ul.FuY.Q.2016Advances in nanostructured thin film materials for solar cell applicationsRenewable and Sustainable Energy Reviews5972673710.1016/j.rser.2015.12.268Search in Google Scholar

Charef, A., Benramache, S., Aoun, Y., Benhaoua, B., Lakel, S., Marrakchi, M. (2019): Effect of Substrate Temperature on the Growth and Properties of Nanocrystalline NiO Thin Films. Journal of Nanoelectronics and Optoelectronics, 14, pp. 1667–1671.CharefA.BenramacheS.AounY.BenhaouaB.LakelS.MarrakchiM.2019Effect of Substrate Temperature on the Growth and Properties of Nanocrystalline NiO Thin FilmsJournal of Nanoelectronics and Optoelectronics141667167110.1166/jno.2019.2674Search in Google Scholar

Aoun, Y., Marrakchi, M., Benramache, S., Benhaoua, B., Lakel, S., Charef, A. (2018): Preparation and Characterizations of Monocrystalline Na Doped NiO Thin Films. Materials Research, 21(2), pp. 1–5.AounY.MarrakchiM.BenramacheS.BenhaouaB.LakelS.CharefA.2018Preparation and Characterizations of Monocrystalline Na Doped NiO Thin FilmsMaterials Research2121510.1590/1980-5373-mr-2017-0681Search in Google Scholar

Sharma, R., Acharya, A.D., Shrivastava, S.B., Patidar, M.M., Gangrade, M., Shripathi, T., Ganesan, V. (2016): Studies on the structure optical and electrical properties of Zn-doped NiO thin films grown by spray pyrolysis. Optik, 127(11), pp. 4661–4668.SharmaR.AcharyaA.D.ShrivastavaS.B.PatidarM.M.GangradeM.ShripathiT.GanesanV.2016Studies on the structure optical and electrical properties of Zn-doped NiO thin films grown by spray pyrolysisOptik127114661466810.1016/j.ijleo.2016.01.050Search in Google Scholar